metricas
covid
Buscar en
Boletín de la Sociedad Española de Cerámica y Vidrio
Toda la web
Inicio Boletín de la Sociedad Española de Cerámica y Vidrio Study of the structural, ferroelectric and dielectric properties of BaTiO3 co-do...
Información de la revista
Vol. 62. Núm. 3.
Páginas 284-291 (mayo - junio 2023)
Compartir
Compartir
Descargar PDF
Más opciones de artículo
Visitas
2522
Vol. 62. Núm. 3.
Páginas 284-291 (mayo - junio 2023)
Acceso a texto completo
Study of the structural, ferroelectric and dielectric properties of BaTiO3 co-doped with Sn4+ and Cr3+
Estudio de las propiedades estructurales, ferroeléctricas y dieléctricas de BaTiO3 co-dopado conSn4+ y Cr3+
Visitas
2522
Fernando Daniel Cortés-Vega, Carlos Montero-Tavera, Jose Martin Yañez-Limón
Autor para correspondencia
jmyanez@cinvestav.mx

Corresponding author.
Center for Research and Advanced Studies of the National Polytechnic Institute, Querétaro Unit, Libramiento Norponiente No. 2000 Fracc. Real de Juriquilla, Querétaro, Qro., 76230 Querétaro, Mexico
Este artículo ha recibido
Información del artículo
Resumen
Texto completo
Bibliografía
Descargar PDF
Estadísticas
Figuras (6)
Mostrar másMostrar menos
Tablas (3)
Table 1. Parameters obtained by Rietveld refinement.
Table 2. Values of remnant and maximum polarization for processed samples.
Table 3. Energy storage density.
Mostrar másMostrar menos
Material adicional (1)
Abstract

In the present work, we studied the effect of Sn4+ and Cr3+ doping on the structural, ferroelectric, and dielectric properties of BaSnxCryTi1−(x+y)O3. The materials were prepared by a combination of high-energy mechanical milling and solid-state reactions. The X-Ray Diffraction (XRD) analysis and Rietveld refinements confirmed the presence of a single tetragonal phase for the pure and doped samples. The SEM study revealed that the microstructure is highly susceptible to the addition of both dopants, causing an evident grain refinement. On the other hand, the addition of Sn4+ and Cr3+ had a strong influence on ferroelectric properties, as observed by the pinching of the ferroelectric hysteresis loops. The addition of Sn4+ increases the remnant and maximum polarization, as the Cr3+ doping promoted the contrary effect. Co-doping with Sn4+ and Cr3+ resulted in a maximum energy storage value of 0.2574J/cm3 with a efficiency of up to 65%, overcoming the values of pure BT. The relative permittivity of all doped samples remained in values of ∼1000, just a little below the permittivity of pure BT.

Keywords:
Co-doping
Ferroelectric properties
Dielectric properties
Structural properties
Resumen

En el presente trabajo se estudiaron los efectos del co-dopaje con Sn4+ y Cr3+ en las propiedades estructurales, ferroeléctricas y dieléctricas de BaSnxCryTi1-(x+y)O3. Los materiales se prepararon mediante una combinación de molienda mecánica de alta energía y reacciones en estado sólido. Los análisis de difracción de rayos X (DRX) y los refinamientos Rietveld confirmaron la presencia de únicamente la fase tetragonal tanto en la muestra de BT puro como en las dopadas. Los estudios realizados por microscopia electrónica de barrido revelaron que la microestructura de los materiales fabricados es altamente susceptible a la adición de ambos dopantes, provocando un refinamiento considerable de tamaño de grano. Por otro lado, el dopaje con los iones Sn4+ y Cr+3 demostró tener una fuerte influencia en las propiedades ferroeléctricas, como se observó mediante la contracción de los ciclos de histéresis ferroeléctrica. La adición de Sn4+ incrementó los valores de polarización remanente y máxima, mientras que el dopaje con Cr3+ promovió el efecto contrario. El co-dopaje con Sn4+ y Cr3+ dio como resultado un valor máximo de almacenamiento de energía de 0,2574J/cm3 con una eficiencia de 65%, superando los valores de BT puro. La permitividad relativa de las muestras dopadas se mantuvo en valores de ∼1000, mostrando un decremento mínimo en comparación a la permitividad del BT puro.

Palabras clave:
Co-dopaje
Propiedades ferroeléctricas
Propiedades dieléctricas
Propiedades estructurales
Texto completo
Introduction

Nowadays, the use of ferroelectric ceramic materials to develop new technologies is an area of deep interest in the scientific and industrial sectors. The use of this class of materials is very wide, ranging from sensors and actuators to energy conversion and catalysis [1–3]. Furthermore, the use of lead-free ferroelectrics has attracted attention in the field of energy storage and more specifically, in advanced pulsed power capacitors due to their ability to release a high power density in a fast charge–discharge [4,5].

BaTiO3 is one of the most important lead-free ferroelectric materials, and therefore, it has been the subject of several studies. Searching for the enhancement of the properties of BaTiO3, it has been doped with multiple elements such as Bi, Fe, Li, Y, Nb, and Cr, as well as different rare-earth ions [6–12]. Particularly, Cr doped BaTiO3 has been studied in regards to its catalytics properties. Chilukoti Srilakshmi et al. [13] synthesized BaTiO3 doped with chromium by conventional oxalate and microwave assisted hydrothermal synthesis, achieving an improved performance in the conversion of nitrobenzene. Similar studies were carried out by I. C. Amaechi et al. [14] that reported on the synthesis of BaTiO3 doped with Cr3+ in a range of 2–8mol% by microwave-assisted method. Here was demonstrated the improvement in the photocatalytic performance of doped BaTiO3 by photodegradation assessment of methyl orange, being ∼2.7 times higher than for the undoped material. Relevant results reported in the literature show that the incorporation of Cr in the BT allows maintaining the tetragonal structure up to concentrations in an atomic fraction of 0.03, and from 0.04 a pseudocubic phase can appear. On the other hand, the multivalent nature of Cr has also been detected when doping BT, found in Cr3+ and Cr5+ oxidation states [15].

The synthesis method is very important in the final crystalline structure of BT nanoparticles doped with Cr. C. Srilakshmi et al. [13] found that it is possible to obtain doped BT nanoparticles with Cr up to a concentration of 0.05 with a tetragonal or cubic structure, depending on whether a conventional oxalate hydrothermal method or a microwave-assisted method is used. The XPS results of the same authors show that oxidation states of Cr in BT matrix can occur in Cr3+ and Cr6+. Additionally, studies of first principles by DFT [16] predict that Cr doping of the BT in its cubic phase should lead to an increase in the volume of the unit cell, in the brittleness of the ceramic, and a decreasing trend in the band-gap of the BT.

On the other hand, Tao Shi et al. [17] analyzed the influence of Sn4+ doping in BaTiO3 by means of high resolution scanning transmission electron microscopy and first principles calculations. They determined that the presence of Sn4+ is responsible for the strong enhancement of dielectric permittivity and the presence of a diffuse phase transition in the doped material. Other researchers have also reported large enhancements of the piezoelectric and dielectric performance obtained by doping with Sn4+[18,19].

W. Liu et al. [16] emphasize the general characteristics of the phase diagram of Sn-BaTiO3. Among the effects of the doped BT with Sn are the decrease in TC and the increase in the transition temperatures R–O and O–T. In such a way that for a concentration close to 11% of Sn, the 4 crystalline phases of BT coexist, R, O, T, and C, called quadruple point.

N. Horchidan et al. [20] studied the effects of BT doped with Sn, using several characterization techniques, finding that for concentrations less than 0.15 the tetragonal phase is obtained, and for concentrations greater than or equal to 0.20 the cubic phase is obtained. Additionally, the dielectric and Raman spectroscopy results indicate that at concentrations of 0.05 there is a coexistence of phases O and T, and at 0.15 there is a coexistence of T and C phases. Also, the introduction of Sn induces the appearance of polar nano-regions related to the relaxor behavior of the BST system. Li et al. [21] reported the synthesis of BT doped with Sn under an H2–N2 mixture atmosphere, obtaining a very large dielectric constant at room temperature (1.2×104 at 1kHz), as well as dielectric losses close to 1% and resistivities of the order of tens of MΩcm.

However, to the best of our knowledge the combination of these dopants has not been reported previously, and therefore, there is no information about the behavior and properties of this co-doped system.

In this work, we present the study of ferroelectric, dielectric and structural properties of BaTiO3 (BT) co-doped with Sn4+ and Cr3+, as well as the analysis of the evolution of the ferroelectric–paraelectric transition from a typical Curie-Weiss behavior to partial diffuse transition. The obtained results represent novel and useful information for the development and better understanding of new ferroelectric systems.

Experimental procedureMaterials

Barium carbonate (BaCO3; ≥99% purity), titanium dioxide (TiO2; 99.5% purity), tin oxide (SnO2; 99.9% purity) and chromium oxide (Cr2O3; ≥98%) were purchased from Sigma–Aldrich.

Processing and synthesis

The starting powders were mixed using a high-energy mill SPEX 8000 according to the following compositions: BaTiO3 (BT), BaCr0.01Ti1−(0.01)O3 (BCT1), BaCr0.03Ti1−(0.03)O3 (BCT3), BaSn0.02Cr0.01Ti1−(0.03)O3 (BSCT1), BaSn0.02Cr0.03Ti1−(0.05)O3 (BSCT3) and BaSn0.02Cr0.00Ti1−(0.02)O3 (BST). The milling time for each composition was 2h, using zirconia balls with different diameters. The ratio of zirconia balls was 2:10 with diameters of 10 and 6mm, respectively. The mixtures of powders resulting from the milling stages were calcined at 1100°C for 2h, and then, grinded in a mortar and compacted in cylindrical pellets of 10mm of diameter at a pressure of 193.11MPa. The cylindrical pellets were densified at 1300°C for 2h in air atmosphere. After sintering, the density of all samples was estimated by Archimedes principle.

Characterization

The crystalline structure of the prepared materials was analyzed using a Rigaku Dmax-2100 diffractometer with a Bragg–Brentano geometry and Cu-Kα radiation (λ=1.5418Å) at step size=0.02, t=0.3s, and 20°–70° in 2θ range. The study of the surface microstructure was carried out with a field emission Philips XL30 ESEM microscope working at 15kV and with secondary electrons detector. All the samples were previously polished and coated with a thin layer of gold, using a coater machine Denton Vacuum desk V.

The grain size was calculated by measuring the diameter of 100 single grains for each sample using the free software ImageJ. Ferroelectric characterization was performed using an equipment from Radiant Technologies Inc. with a coupled external high-voltage amplifier (4000V) TREK model 609-6 at 200Hz (5ms) and using a triangle waveform. The dielectric properties were measured with a KEYSIGHT E499A impedance analyzer operating at a frequency range of 20Hz to 10MHz. The impedance analyzer is coupled to a homemade oven that allows temperature measurements in a range of 25–300°C.

Results and discussion

Fig. 1a–d shows the XRD patterns, lattice parameters and relative density of the investigated samples. The XRD patterns for all the investigated samples are shown in Fig. 1a. The Rietveld refinement made using the software MAUD [22] confirmed the presence of a single tetragonal phase for all sample compositions, the Rwp values obtained in the fitting to XRD patterns of our set of samples are in a range between 17 and 24%, and sigma values are between 2.18 and 2.45. In Table 1 are listed the resulting parameters of the Rietveld refinement for all the studied samples. In addition, the good fitting achieved from the Rietveld Refinement for the sample BT can be found in the supplementary material (see Fig. S1). Further evidence of the presence of a tetragonal phase may be observed in Fig. 1a. Here, we can see the presence of the characteristic tetragonal planes (002) and (200) for all the processed samples [23] PDF#05-0626. The evolution of the lattice parameters with doping is observed in Fig. 1c. On the one hand, the parameter cT tends to slightly decrease with doping when compared with pure BT. In contrast, the parameter aT increases with doping, and therefore, decreases the tetragonality degree. The relative density for each sample is observed in Fig. 1d. The obtained values suggest that the addition of doping atoms hinders the densification process to a certain degree as we observe a decrease in the relative density in all cases, except by the sample BCT1. The highest relative density was observed for pure BT (97.3%), whereas the lowest density values were found for the sample BCT3 (83.8%).

Fig. 1.

(a) XRD patterns in the 2θ range of 20–70°, (b) amplification of XRD patterns in the range of 44–46°, (c) lattice parameters estimated by Rietveld refinement and (d) relative density measurements.

(0.48MB).
Table 1.

Parameters obtained by Rietveld refinement.

BT  BST  BCT1 
sigma=2.458  sigma=2.251  sigma=2.293 
Rwp (%)=21.37  Rwp (%)=24.35  Rwp (%)=19.32 
Rb (%)=17.355  Rb (%)=18.25  Rb (%)=14.87 
Rexp (%)=8.69  Rexp (%)=10.82  Rexp (%)=8.43 
a=3.9936±6.3E−4  a=3.9973±7.9E−4  a=3.9918±4.6E−4 
c=4.0339±7.4E−4  c=4.0283±9.7E−4  c=4.0296±5.8E−4 
BCT3  BSCT1  BSCT3 
sigma=2.231  sigma=2.189  sigma=2.2814 
Rwp (%)=17.35  Rwp (%)=18.73  Rwp (%)=20.44 
Rb (%)=13.25  Rb (%)=14.33  Rb (%)=15.82 
Rexp (%)=7.77  Rexp (%)=8.55  Rexp (%)=8.96 
a=3.9942±5.1E−4  a=4.0009±4.9E−4  a=4.0026±5.7E−4 
c= 4.0295±6.2E−4  c=4.0264±6.6E−4  c=4.0226±9.1E−4 

In Fig. 2 the SEM images of pure and doped materials are displayed, which correspond to the surface of the as densified samples. Comparatively, all doped samples exhibit a significant grain refinement to a different extent, according to the amount and type of dopant added. The grain size measurements were carried out by measuring the diameter of the grains. Likewise, the average values are plotted in Fig. 3. The sample with the largest grain size was BT with an average diameter of 98.8±15μm, whereas the samples that showed the lowest diameter values were BCT3 and BSCT3, with diameter of 4.6±1.5 and 2.6±0.5μm.

Fig. 2.

SEM images of surface microstructure for pure and doped samples. (a) BT, (b) BST, (c) BCT1, (d) BCT3, (e) BSCT1, and (f) BSCT3.

(1.05MB).
Fig. 3.

Grain size measurements.

(0.09MB).

The relative permittivity of samples is plotted in Fig. 4 in a temperature range of 25–300°C. The maximum relative permittivity point that belongs to the ferroelectric–paraelectric (F–P) transition shows slight shifts to a lower temperature with the addition of dopants. These shifts exhibit a maximum value for the samples BSCT1 and BSCT3, being 113.17 and 113.34°C, respectively. However, the most prominent effect of temperature reduction on the F–P transition is attributed to the single addition of Sn4+ in the BST sample, whereas the influence of Cr3+ is minimal. In good agreement with our results, we observed that the addition of Sn decreases the temperature of the F–P transition. Md. Jawed and Shail Upadhyay [24], studied the effect of 0.05 and 0.15 additions of Sn into the BaTiO3 structure. They reported significant reductions of the F–P temperature going from 123°C for pure BaTiO3 and up to 10°C for the sample with higher amount of Sn. Similar trends were observed by C. Kajtoch in his study of the dielectric properties of BaTiSnO3 ceramics. Here, it was observed that the increase of Sn concentration in the range of 0.05–0.20 (molar fraction) strongly lowers the F–P transition [25]. Remarkably, the relative permittivity before the temperature transition remains very similar among pure and doped samples, without showing a significant reduction. Here, we can see that pure BT has a relative permittivity around 1200 before the F–P transition, whilst the BST, BCT3, and BSCT3 samples exhibit similar values above 1000. The samples with the lowest concentrations of dopants (BCT1 and BSCT1) show a slight decrease in the relative permittivity values. The dispersion of relative permittivity as a function of frequency may be explained in terms of interfacial polarization. Here, we consider that the volume of the grains is a conductive zone that allows the free flow of charges under the influence of an external electrical field, whereas the grain boundaries may be seen as poor or null conductive zones [26–28]. Therefore, free charges move readily in the inner of the grains and accumulate on the grain boundaries, generating an interfacial polarization. Thus, when the applied field is of low frequency, the movement of charges takes place readily, whereas, with the increase of frequency, the free charges are not able to follow the applied electric field.

Fig. 4.

Relative permittivity (ɛ′) measurements of processed samples at different frequencies. (a) BT, (b) BST, (c) BCT1, (d) BCT3, (e) BSCT1 and (f) BSCT3.

(0.66MB).

In the supplementary material, the behavior analysis of the dielectric function with temperature is presented in terms of the Curie Weiss and Uchino-Nomura models. Through the latter, it is possible to determine the degree of diffuseness of the F–P transition, Figs. S1, and S2. The parameters obtained are presented in table S1. The results show that the highest values of diffuseness coefficient (γ) were obtained for the samples BSCT1 and BSCT3, being 1.4458±0.0115 and 1.6143±0.0143, respectively. The high values of γ for the samples BSCT1 and BSCT3 are attributed to the type and concentration of added dopants that generates fluctuations in the chemical composition, formation of crystal defects, and therefore, an increase of the structural disorder that leads to the formation of a broad or diffuse phase transition [20].

The results of dielectric losses are shown in the supplementary material Fig. S3. It can be seen that the dielectric losses are less than 0.5 in all the samples up to 200°C. At higher temperatures an increase in dielectric losses is observed, reaching values close to 1.5 for the BT and BST samples, the samples with Cr do not exceed 0.3 at 300°C. This increase in dielectric losses can be associated with the thermal activation of the different types of defects present in the samples, such as oxygen vacancies and charge imbalance sites due to the presence of Cr3+ and possibly Cr6+. However, the fact that they are lower in samples with Cr is also an indication that in this range of low dopant concentrations, the action of the dopant is to compensate for the native vacancies of oxygen present in BT and BST.

The behavior of the ferroelectric hysteresis loops for all the samples is presented in Fig. 5. Here, we can appreciate the strong influence of Sn4+ and Cr3+ co-doping on the ferroelectric properties. Initially, the pure BT observed in Fig. 4a shows a typical ferroelectric hysteresis loop with values of 10.7μC/cm2 and 21.07μC/cm2 for the remnant (Pr) and maximum (Pmax) polarization, respectively. Comparatively, the addition of Sn4+ in the sample BST0 boosted the value of Pr up to 12.02μC/cm2 but slightly deteriorated the Pmax (see Table 2). Similar results have been found in previous reports, showing increments of Pr with the addition of Sn4+, maintaining a typical ferroelectric hysteresis loop [18,29]. Except for sample BST, all other compositions show a strong reduction of remnant polarization (see Table 2). The addition of Cr3+ promoted the appearance of double hysteresis loops as observed in Fig. 5b and c for samples BCT1 and BCT3, respectively. With the increase of the Cr3+ concentration from BCT1 to BCT3, there is a constriction of the hysteresis loops, as well as a considerable reduction in Pr and Pmax. We consider that the pinched form of the hysteresis loops observed in samples doped with Cr is very likely to be related to local charged defects induced by Cr3+ that replaces Ti and causes imbalances of charge in the oxygen octahedron. Additionally, it has also been reported that Cr may be also present as Cr5+ and Cr6+ oxidation states [13,15], which would induce larger amount of defects. The presence of Cr3+ and Cr6+ together have a similar effect to that observed for Pb–O in PZT, which act as pinning centers of the domain walls and give rise to the pinched shape of the hysteresis loops. We rule out a dominant contribution of Sn-induced polar nano regions, since a low concentration of Sn, 0.02 in atomic fraction, is used in all samples, and in this concentration range the relaxor effects associated with Sn are not expected.

Fig. 5.

Ferroelectric hysteresis loops for pure BT and doped samples measured at a frequency of 200Hz.

(0.65MB).
Table 2.

Values of remnant and maximum polarization for processed samples.

Sample  Pr  Pmax  Sample  Pr  Pmax 
BT  10.7  21.07  BST  12.02  19.2 
BCT1  4.05  16.75  BSCT1  4.39  17.27 
BCT3  1.44  14.32  BSCT3  2.26  15.85 

In general, it is observed that the addition of only Sn4+ enhances the value of Pmax as the addition of Cr3+ decreases the Pr, promoting the formation of slim loops. Given the characteristic of presenting low values of Pr, it is interesting to estimate the recoverable energy storage capacity and storage efficiency [30] for all materials as displayed in Table 3.

Table 3.

Energy storage density.

Sample  Energy storage density (J/cm3Efficiency (%) 
BT  0.1609  35 
BST  0.1130  31 
BSCT1  0.1814  49 
BSCT3  0.2574  65 
BCT1  0.1565  40 
BCT3  0.1724  56 

The highest values of recoverable energy storage and efficiency were found for BSCT3 sample, being 0.2574J/cm3 and 65%, respectively. These values represent a significant improvement in comparison to those observed for pure BT (Energy storage density=0.1609J/cm3 and Storage efficiency=35%). However, the energy storage capacities calculated in this work are lower than others observed for systems as Bi0.5Na0.5TiO3–BaTiO3–SrTi0.875Nb0.1O3, Pb(Zr0.95Ti0.05)0.98Nb0.02O3 and 0.9Pb(Mg1/3Nb2/3)O3–0.1PbTiO3 that have reported values of 1.17 [31], 3.0 [32] and 9.8J/cm3[33], respectively.

Conclusions

In this study, the results of the ferroelectric, dielectric, and structural characterization of the lead-free ferroelectric BaTiO3 co-doped with Sn4+ and Cr3+ have been reported. The addition of both dopants demonstrated to have a strong influence on the physical properties of the host structure. It was observed that the microstructure of doped samples suffered a notable grain refinement and, at the same time, the XRD analysis revealed the presence of a single tetragonal phase for all compositions. The pinching effect of the ferroelectric hysteresis loops might be associated to local charged defects induced by the addition of Cr that is likely to be present in different valence states. The energy storage density and efficiency of the samples increased in all cases except for the sample BST, achieving the best performance for the sample BSCT3.

Acknowledgements

This work was financially supported by the Projects CB 240460, LIDTRA LN2015-254119, and LN2021-315906 of CONACYT. The authors thank the National Laboratory, LIDTRA, for the infrastructure facilities provided for the realization of this work. F.D. Cortes Vega and C. Montero-Tavera are grateful to CONACYT for the scholarships granted for postdoctoral stays and doctoral studies, respectively. Also, the authors want to thank the support provided by the laboratory technicians, Adair Jimenez Nieto, Rivelino Flores Farias, Martín Adelaido Hernández Landaverde, and Agustín Galindo Sifuentes.

Appendix A
Supplementary data

The following are the supplementary data to this article:

References
[1]
A.K. Bain, P. Chand.
Ferroelectric ceramics: devices and applications.
Ferroelectrics, (2017), pp. 195-306
[2]
I. Chilibon, J.N. Marat-Mendes.
Ferroelectric ceramics by sol–gel methods and applications: a review.
J. Sol-Gel Sci. Technol., 64 (2012), pp. 571-611
[3]
R. Whatmore.
Ferroelectric materials.
Springer Handbook of Electronic and Photonic Materials, pp. 1 http://dx.doi.org/10.1007/978-3-319-48933-9_26
[4]
K. Han, N. Luo, S. Mao, F. Zhuo, L. Liu, B. Peng, X. Chen, C. Hu, H. Zhou, Y. Wei.
Ultrahigh energy-storage density in A-/B-site co-doped AgNbO3 lead-free antiferroelectric ceramics: insight into origin of antiferroelectricity.
J. Mater. Chem. A, 3 (2019), pp. 1-9
[5]
H. Pan, Y. Zeng, Y. Shen, Y.H. Lin, J. Ma, L. Li, C.W. Nan.
BiFeO3–SrTiO3 thin film as a new lead-free relaxor-ferroelectric capacitor with ultrahigh energy storage performance.
J. Mater. Chem. A, 5 (2017), pp. 5920-5926
[6]
W.B. Li, D. Zhou, L.X. Pang, R. Xu, H.H. Guo.
Novel barium titanate based capacitors with high energy density and fast discharge performance.
J. Mater. Chem. A, 5 (2017), pp. 19607-19612
[7]
Z. Shen, X. Wang, B. Luo, L. Li.
BaTiO3–BiYbO3 perovskite materials for energy storage applications.
J. Mater. Chem. A, 3 (2015), pp. 18146-18153
[8]
M.J. Wang, H. Yang, Q.L. Zhang, Z.S. Lin, Z.S. Zhang, D. Yu, L. Hu.
Microstructure and dielectric properties of BaTiO3 ceramic doped with yttrium, magnesium, gallium and silicon for AC capacitor application.
Mater. Res. Bull., 60 (2014), pp. 485-491
[9]
J. Huang, J. Zhang, H. Yu, M. Wei, H. Chen, C. Yang.
Improvement of dielectric and energy storage properties in BaTiO3 ceramics with BiNbO4 modified.
Ferroelectrics, 510 (2017), pp. 8-15
[10]
H.T. Langhammer, T. Müller, R. Böttcher, H.P. Abicht.
Structural and optical properties of chromium-doped hexagonal barium titanate ceramics.
J. Phys. Condens. Matter, 20 (2008),
[11]
S. Madolappa, R. Sagar, R.L. Raibagkar.
Synthesis, structural and electrical investigations of Gd-and Cr-Doped BaTiO3 nanoparticle ceramics.
Ferroelectrics, 413 (2011), pp. 37-45
[12]
J. Shah, R.K. Kotnala.
Induced magnetism and magnetoelectric coupling in ferroelectric BaTiO3 by Cr-doping synthesized by a facile chemical route.
J. Mater. Chem. A, 1 (2013), pp. 8601-8608
[13]
C. Srilakshmi, R. Saraf, V. Prashanth, G.M. Rao, C. Shivakumara.
Structure and catalytic activity of Cr-doped BaTiO3 nanocatalysts synthesized by conventional oxalate and microwave assisted hydrothermal methods.
Inorgan. Chem., 55 (2016), pp. 4795-4805
[14]
I.C. Amaechi, G. Kolhatkar, A.H. Youssef, D. Rawach, S. Sun, A. Ruediger.
B-site modified photoferroic Cr3+-doped barium titanate nanoparticles: microwave-assisted hydrothermal synthesis, photocatalytic and electrochemical properties.
RSC Adv., 9 (2019), pp. 20806-20817
[15]
D.-Y. Lu, Y. Liang.
Valence states and dielectric properties of fine-grained BaTiO3 ceramics co-doped with double valence-variable europium and chromium.
Ceram. Int., 44 (2018), pp. 14717-14727
[16]
K.M. Hossain, S. Ahmad, S.K. Mitro.
Physical properties of chromium-doped barium titanate: effects of chromium incorporation.
Phys. B: Condens. Matter, 626 (2022), pp. 413494
[17]
T. Shi, L. Xie, L. Gu, J. Zhu.
Why Sn doping significantly enhances the dielectric properties of Ba(Ti1−xSnx)O3.
Sci. Rep., 5 (2015), pp. 8-11
[18]
W. Liu, J. Wang, X. Ke, S. Li.
Large piezoelectric performance of Sn doped BaTiO3 ceramics deviating from quadruple point.
J. Alloys Compd., 712 (2017), pp. 1-6
[19]
S. Gattu, K.S. Dasari, V.R. Kocharlakota.
Structural and dielectric properties of sn doped barium magnesuim zirconium titanate perovskite ceramics.
World J. Condens. Matter Phys., 05 (2015), pp. 346-352
[20]
N. Horchidan, A.C. Ianculescu, C.A. Vasilescu, M. Deluca, V. Musteata, H. Ursic, R. Frunza, B. Malic, L. Mitoseriu.
Multiscale study of ferroelectric–relaxor crossover in BaSnxTi1−xO3 ceramics.
J. Eur. Ceram. Soc., 34 (2014), pp. 3661-3674
[21]
L. Li, R. Wang, S. Yu, Z. Sun, H. Zheng.
Novel tin-doped BaTiO3 ceramics with non-reducibility and colossal dielectric constant.
Mater. Lett., 220 (2018), pp. 119-121
[22]
M. Ferrari, L. Lutterotti.
Method for the simultaneous determination of anisotropic residual stresses and texture by X-ray diffraction.
J. Appl. Phys., 76 (1995), pp. 7246-7255
[23]
D.-H. Yoon.
Tetragonality of barium titanate powder for a ceramic capacitor application.
J. Ceram. Process. Res., 7 (2006), pp. 343-354
[24]
M.J. Ansaree, S. Upadhyay.
Study of phase evolution and dielectric properties of Sn-doped barium titanate.
Emerg. Mater. Res., 6 (2017), pp. 21-28
[25]
C. Kajtoch.
Dielectric properties of Ba (Ti1−xSnx)O3 ceramics in the paraelectric phase.
Ceram. Int., 37 (2011), pp. 387-391
[26]
J. Sharma, J. Parashar, V.K. Saxena, D. Bhatnagar, K.B. Sharma.
Study of dielectric properties of nanocrystalline cobalt ferrite upto microwave frequencies.
Macromol. Symp., 357 (2015), pp. 38-42
[27]
S.A. Mazen, N.I. Abu-elsaad.
Structural, magnetic and electrical properties of the lithium ferrite obtained by ball milling and heat treatment.
Appl. Neurosci., 3 (2015), pp. 105-114
[28]
C. Rayssi, S. El Kossi, J. Dhahri, K. Khirouni.
Frequency and temperature-dependence of dielectric permittivity and electric modulus studies of the solid solution Ca0.85Er0.1Ti1−xCo4x/3O3 (0x0.1).
RSC Adv., 8 (2018), pp. 17139-17150
[29]
S.K. Upadhyay, P. Bag.
Electro-caloric effect in lead-free Sn doped BaTiO3 ceramics at room temperature and low applied fields Electro-caloric effect in lead-free Sn doped BaTiO3 ceramics at room temperature and low applied fields Sanjay Kumar Upadhyay.
V. Raghavendra Reddy, (2014),
[30]
L. Zhao, Q. Liu, S. Zhang, J.F. Li.
Lead-free AgNbO3 anti-ferroelectric ceramics with an enhanced energy storage performance using MnO2 modification.
J. Mater. Chem. C, 4 (2016), pp. 8380-8384
[31]
J. Shi, X. Liu, W. Tian.
High energy-storage properties of Bi0.5Na0.5TiO3–BaTiO3–SrTi0.875Nb0.1O3 lead-free relaxor ferroelectrics.
J. Mater. Sci. Technol., 34 (2018), pp. 2371-2374
[32]
S.I. Shkuratov, J. Baird, V.G. Antipov, S. Zhang, J.B. Chase.
Multilayer PZT 95/5 antiferroelectric film energy storage devices with giant power density.
Adv. Mater., 31 (2019), pp. 1904819
[33]
M. Sadl, O. Condurache, A. Bencan, M. Dragomir, U. Prah, B. Malic, M. Deluca, U. Eckstein, D. Hausmann, N.H. Khansur, K.G. Webber, H. Ursic.
Energy-storage-efficient 0.9Pb(Mg1/3Nb2/3)O3−0.1PbTiO3 thick films integrated directly onto stainless steel.
Acta Mater., 221 (2021), pp. 117403
Copyright © 2022. The Author(s)
Descargar PDF
Opciones de artículo