covid
Buscar en
Journal of Applied Research and Technology. JART
Toda la web
Inicio Journal of Applied Research and Technology. JART Room-temperature ferromagnetism in Ni-doped TiO2 diluted magnetic semiconductor ...
Información de la revista
Vol. 15. Núm. 2.
Páginas 132-139 (abril 2017)
Compartir
Compartir
Descargar PDF
Más opciones de artículo
Visitas
6150
Vol. 15. Núm. 2.
Páginas 132-139 (abril 2017)
Original
Open Access
Room-temperature ferromagnetism in Ni-doped TiO2 diluted magnetic semiconductor thin films
Visitas
6150
Bushra Parveena,b, Mahmood-ul-Hassana,
Autor para correspondencia
mahmood.physics@pu.edu.pk

Corresponding author.
, Zeeshan Khalida, Saira Riazc, Shahzad Naseemc
a Materials Growth and Simulation Laboratory, Department of Physics, University of the Punjab, Lahore 54590, Pakistan
b Department of Physics, Lahore Garrison University, Lahore 54590, Pakistan
c Centre of Excellence in Solid State Physics, University of the Punjab, Lahore 54590, Pakistan
Este artículo ha recibido

Under a Creative Commons license
Información del artículo
Resumen
Texto completo
Bibliografía
Descargar PDF
Estadísticas
Figuras (6)
Mostrar másMostrar menos
Tablas (2)
Table 1. The lattice constants, crystallite size and strain calculated from XRD patterns.
Table 2. The remanent magnetization, saturation magnetization and coercivity extracted from the measured hysteresis loops.
Mostrar másMostrar menos
Abstract

We report undoped and Ni-doped TiO2 (xNi=0.00, 0.50, 1.00, 1.50, 2.00 and 2.50wt.%) thin films fabricated on glass substrates by using a combination of solid-state reaction and dip coating techniques. The structural properties are observed by X-ray diffraction (XRD), which have depicted that annealing at 650°C results in rutile Ni-doped TiO2 as a major phase along with a minor anatase phase. The surface morphology of the deposited thin films, as measured by scanning electron microscopy (SEM), indicates granular spherical shaped nanostructures. Room-temperature ferromagnetism (RTFM) has been illustrated by all the grown thin films, as elucidated by vibrating sample magnetometer (VSM). Although Ni content has no pronounced effect on the crystallinity that indicates a substitutional replacement of Ni in TiO2 lattice, however, Ni content is observed to influence the ferromagnetic behavior. Therefore, the present study signifies the potential spintronic applications of Ni-doped TiO2 diluted magnetic semiconductors, fabricated by a low-cost method, as it exhibits RTFM with nanograins at the surface.

Keywords:
Diluted magnetic semiconductors
Dip coating
Solid-state reaction
Room-temperature ferromagnetism (RTFM)
Vibrating sample magnetometer
Texto completo
1Introduction

In the last few years, thin film technology has been playing a vital role in the fabrication of solid-state magnetic storage devices to study and realize novel phenomena to meet the requirements of the integrated-circuit industry. The cost of fabrication of thin films is very low as compared to that of their bulk counterparts. Moreover, the charge transport and the information storage can effectively be realized in nanoscale devices by employing thin films. Diluted magnetic semiconductors have a prominent place in traditional semiconductor-based spintronic research. Traditional semiconductors, doped with a small concentration of magnetic ions to associate magnetic degree of freedom, have become suitable for both current controlling and magnetic storage device applications (Oganisian, Hreniak, Sikora, Gaworska-Koniarek, & Iwan, 2015; Paulauskas et al., 2013). TiO2 doped with various magnetic ions for achieving room-temperature ferromagnetism (RTFM) is one of the attractive aspects in spintronics research. Basically, TiO2 appears in three different crystallographic phases namely, anatase, rutile and brookite. Among which rutile phase is the preferred one. Rutile phase has been widely studied, as it is non toxic with high transparency in the visible region, it has high refractive index, high dielectric constant and good chemical stability (Oganisian et al., 2015; Paulauskas et al., 2013; Sahdan, Nayan, Dahlan, Mahmoud, & Hashim, 2012); therefore, it is considered as one of the suitable photocatalysts in heterojunctions. Also, it has potential applications including gas sensors, membranes, LEDs, fibers, light transparent electrodes, heat reflectors and optical gain media (Akpan & Hameed, 2010; Chen, Yang, Wang, & Jiang, 2006). There are many reports in the literature, which indicates that the band gap of TiO2 can be tapered by doping with transition metals (Fe, Cr, Mn, Ni), nonmetals (F, I, P, N, S), rare earth elements (La, Gd, Nd, Er, Pr) and alkaline earth metals (Be, Mg) etc., that enhance the photocatalytic activity in the visible light (Ahmad et al., 2010; Al-Jawad, 2014; Asahi, Morikawa, Irie, & Ohwaki, 2014; Ayieko, Musembi, Waita, Aduda, & Jain, 2013; Buzby et al., 2006; Di Valentin, Pacchioni, & Selloni, 2005; Gültekin, 2014; Hamal & Klabunde, 2007; Hermawan, Pranowo, & Kartini, 2011; Hernández-Martínez, Estevez, Vargas, Quintanilla, & Rodríguez, 2012; Li, Ding, Liu, & Ning, 2013; Niemela, Yamauchi, & Karppinen, 2014; Seery, George, Floris, & Pillai, 2007; Sobana, Muruganadham, & Swaminathan, 2006; Tian, Gao, Deng, et al., 2013; Tian, Gao, Kong, et al., 2013; Yang et al., 2007), which indicates potential opto-electronic device applications. A surprising fact is the presence of room-temperature ferromagnetism in undoped TiO2 (Hong, Sakai, Poirot, & Brizé, 2006; Yoon et al., 2006). The ferromagnetism is reported to be originated because of oxygen vacancies acting as n-type dopant and cause a magnetic order. Through theoretical calculation (Paxton & Thien-Nga, 1998) the magnetic ordering has been demonstrated to be originated because of the Ti states operating within the bandgap. Transition metal elements are preferred as dopants because of their almost similar ionic radii with the Ti-cations in the host TiO2 lattice, and additionally mediate ferromagnetism. Among many transition metal ion dopants, Ni+2 is considered to be more efficient dopant in TiO2, as it can improve electrical and magnetic properties (Ayieko et al., 2013; Li et al., 2013; Nosaka, Matsushita, Nishino, & Nosaka, 2005). Oganisian et al., synthesized Fe-doped TiO2 by sol–gel method and studied the effect of doping concentration on the magnetism, and suggested the formation of multi-domain structure that enhances with Fe contents (Oganisian et al., 2015). Choudhary et al., have reported the role of Oxygen defects in assisting paramagnetic to ferromagnetic phase change activated through the Fe doping in TiO2 (Choudhury, Verma, & Choudhury, 2014). Similarly, Ni-doped TiO2 is employed to study the effect of dopants on the ferromagnetic properties of TiO2 stabilized in rutile phase (Park, Choi, Lee, Kim, & Kim, 2007). On the other hand, J. Tian et al. fabricated TiO2 thin films by sol–gel process and observed that increase in transition metal concentration reduces magnetization (Tian, Gao, Deng, et al., 2013; Tian, Gao, Kong, et al., 2013). Gultekin, have studied Au-doped TiO2 thin films, and reported that TiO2 show body centered tetragonal structure, and the band gap of TiO2 thin films increases from 3.74eV to 3.89eV with increase in Au nanoparticle concentrations (Gültekin, 2014). Yang et al. characterized C and V – TiO2 photocatalysts by sol-gel process for degradation of acetaldehyde, and observed that V dopants in TiO2 increases the surface area, making it suitable for light activity (Yang et al., 2007). Similarly, Ni-doped TiO2 thin films prepared by spray pyrolysis have shown that Ni stabilizes TiO2 in rutile phase, making it more efficient in photocatalytic applications (Al-Jawad, 2014). Hermawan et al. (2011) synthesized Ni-doped TiO2 nanocrystals by sol–gel process and observed that the crystallite size increases from 18.51nm to 20.35nm and the band gap energy decreases from 2.73eV to 2.51eV. The study of magnetic character in TiO2 oxide semiconductors is motivated because of recent interesting reports on In2O3, ITO, SnO2, in which magnetic doping induced magnetic properties have been illustrated (Babu & Kaleemulla, 2016; Babu et al., 2016; Borges, Scolfaro, Alves, da Silva, & Assali, 2012; Kuppan et al., 2016a, 2016b; Xu et al., 2009). As it is evident in the literature, no report exist on Ni-doped TiO2 for spintronics applications as DMS, fabricated by low cost method, to exhibit ferromagnetism at room temperature (RT).

In this work, Ni-doped TiO2 thin films are deposited by employing a combination of solid-state reaction and dip coating techniques with a focus on magnetic device applications, with various dopant concentrations (xNi=0.00, 1.00, 1.50, 2.00 and 2.50wt.%). Ni is a suitable transition metal magnetic dopant for TiO2 and this diluted magnetic semiconductor has worth applications in magnetic data storage devices. The structural, morphological and ferromagnetic properties have been explored using XRD, SEM and VSM, respectively. The results obtained are correlated and compared with the literature and significant points have been elaborated with a focus on the utilization of the studied thin films for data storage applications.

2Experimental procedures

In this study, we have employed a very simple and low cost method to prepare Ni-doped (xNi=0.00, 0.50, 1.00, 1.50, 2.00 and 2.50 at wt.%) TiO2 Thin films on glass substrate. For the fabrication of undoped thin film, 3.2g Titanium dioxide powder was added into ethanol solution and stirred using a magnetic stirrer for 1h at 70°C, to achieve a well-mixed and uniform solution. The TiO2 thin film was fabricated onto a glass substrate using dip coating. In this method ultrasonically cleaned glass substrate were dipped into the prepared solution for 2–3 times to get a suitable and uniform thickness of the film. The TiO2 thin film deposited on the glass substrate was dried in an electric oven at 150°C for 15min. In this way one layer of TiO2 was deposited on the glass substrate. This process was repeated 3 times to get appropriate TiO2 layer thickness. Similarly, Ni-doped (xNi=0.50, 1.00, 1.50, 2.00 and 2.50 at wt.%) TiO2 thin films were fabricated by adding appropriate amounts of NiO powders (according to their molar masses) into the TiO2 solution. All the prepared thin films have been annealed in a digital furnace at 650°C for 60min, to enhance the crystallinity. The temperature of 650°C was attained in two steps, from 0°C to 350°C in 90min, and then from 350°C to 650°C in 60min. The crystal structure of thin films is observed with X-ray diffraction (XRD). The surface morphological details are elucidated by employing scanning electron microscopy (SEM). The ferromagnetic behaviors have been studied by vibrating sample magnetometer (VSM).

3Results and discussion3.1Structural study

XRD patterns of undoped and Ni-doped TiO2 (xNi=0 to 2.50wt.%) thin films deposited on glass substrates and annealed in air for 1h at 650°C are shown in Figure 1. The X-rays are diffracted at the angles of 25.2°, 27.4°, 36.1°, 39.2°, 41.3°, 44.1°, 48.1°, 54.4°, 56.7°, 62.8°, 64.1°, 69.1° corresponding to various crystallographic planes, as Figure 1 shows. These XRD patterns are compared with ICDD files for anatase TiO2 (ICDD file number: 21-1272) and rutile TiO2 (ICDD File number: 87-0710). For undoped and Ni-doped titanium dioxide, a major phase of rutile TiO2 is evident; nevertheless, a minor phase of anatase TiO2 is also present for all compositions of Ni. The 2θ peaks around 25.2° and 48.1° belongs to the anatase phase for undoped and Ni-doped TiO2. The smaller content of anatase compared to the rutile phase is evident from diffraction intensities. It can be observed that the anatase phase is not induced because of the Ni addition but it is already present in the precursor powder of TiO2, as shown in Figure 1. The lattice constants a and c have been calculated from the XRD spectra for major rutile phases, using the following relation (Wilso, Matijasevich, Mitchell, Schulz, & Will, 2006)

here d denotes the interplanar distance and h, k, l show the miller indices. The calculated lattice constants a and c, for undoped and Ni-doped TiO2, are displayed in Table 1. The calculated lattice parameters are plotted against Ni-concentration as given in Figure 2. The calculated values lattice constants are in good match with earlier reports. The crystallite size is extracted from the major (110) peak using Debye-Scherer's relation (Kuznetsov et al., 2009)
where D=crystallite size, k=shape factor that is equal to 0.9, λ=X-ray wavelength and β=full width at half maximum (FWHM). The undoped TiO2 thin film has a crystallite size of 17.677nm. Doping with xNi=0.50%, the crystallite size decreases to 15.919nm. When the dopant concentration further increases to 1.00%, the crystallite size value decreases to 15.704nm. The decreasing crystallite size might be justified by the presence of Ni–O–Ti bonds in Ni-doped TiO2, which inhibits the growth of the crystals. Nonetheless, as the Ni concentration increases further to 1.50%, the crystallite size again increases to 19.677nm, and for the last two concentrations 2.00% and 2.50%, the crystallite size again decreases to 18.847nm and 16.823nm. This shows that the Ni+2 ion replaces Ti+4 ions substitutionally and results in linear decay of the crystallite size. The fluctuation in the crystallite size is due to the lattice strains, which are produced during the synthesis of undoped and Ni-doped TiO2. The crystallite size starts to increase when the number of dislocations decreases with the increase in Ni content (Prabbu, Rao, Kumar, & Kumari, 2013; Purushothan & Krishna, 2015; Vijay et al., 2009). The calculated crystallite size is plotted against the Ni content, as shown in Figure 3. Although, the anatase phase is already present in the precursor TiO2 power but the rutile phase stability can also be justified because of the calculated crystallite size that is >14nm, which is a critical value, below and above, it stabilizes the anatase and rutile phases, respectively (Bahadur, Pasricha, G, Chand, & Kotnala, 2012). The strain present in the samples because of lattice imperfections and distortion is calculated by employing Stoke Wilson formula (Wilso et al., 2006)

Fig. 1.

X-ray diffraction patterns of the precursor powder TiO2 and thin films of TiO2 with xNi=0.00, 1.00, 1.50, 2.00 and 2.50%. All the grown thin film samples indicate rutile TiO2 as dominating phase along with a minute contribution from anatase TiO2 phase. However, the presence of the peaks from the anatase phase can be observed from the XRD pattern of the precursor TiO2 powder; therefore, the presence of the anatase phase is not due to Ni addition in TiO2, instead, the anatase phase is already present in the precursor TiO2 powder.

(0.21MB).
Table 1.

The lattice constants, crystallite size and strain calculated from XRD patterns.

xNi  Lattice constantsCrystallite size
(nm) 
Strain (10−3
(%)  a=b (Å)  c (Å)     
0.0  4.600  2.955  17.677  9.046 
0.5  4.645  2.955  15.919  7.254 
1.0  4.582  2.971  15.704  9.012 
1.5  4.616  2.962  19.626  7.860 
2.0  4.616  2.962  18.847  7.240 
2.5  4.633  2.958  16.823  8.200 
Fig. 2.

The lattice parameters a and c, evaluated from XRD patterns of undoped and Ni-doped TiO2 thin films are plotted against the Ni content. The graph shows that with increasing the Ni content the value of lattice constants a and c varies from 4.60Å to 4.63Å and 2.955Å to 2.977Å, respectively.

(0.08MB).
Fig. 3.

Crystallite size calculated from the XRD and W–H analysis and grain size observed by SEM (see Fig. 5) are plotted against the Ni content. The graph shows that with varying the Ni content there is a small fluctuation in the grain size as determined from the SEM images; however, it has an overall decreasing tendency. The crystallite size randomly varies with the Ni content.

(0.15MB).

The undoped TiO2 thin film possesses strain value of 9.046×10−3. Upon doping with xNi=0.50%, strain value decreased to 7.254×10−3. When dopant concentration was further increased to 1.00%, strain value increased to 9.012×10−3. However, as the Ni concentration increased further to 1.50%, associated strain value decreased to 7.86×10−3 and for the last two concentrations 2.00% and 2.50%, strain values are 7.24×10−3 and 8.20×10−3 respectively. The smaller values of strain and dislocation density enhance free carrier mobility in the host lattice. During the thermal energy relaxations within the sample, certain deformations are produced depending on temperature gradient in different directions which is the cause for increase and decrease in strain. Secondly, since strain is inversely related with crystallite size therefore variation in crystallite size will alter the related deformations within the sample (Kuznetsov et al., 2009; Prabbu et al., 2013; Purushothan & Krishna, 2015; Wilso et al., 2006).

The strain values plotted versus Ni content are depicted in Figure 4. Using Williamson–Hall (W–H) plot method, the crystallite size and the strain are further computed. The following equation has been utilized to elucidate the required properties (Patle, Labhane, Huse, & Chaudhari, 2015).

where, D=Crystallite size, ¿=strain. Eq. (3) is called as W–H equation. We have plotted graphs for all concentrations of Ni by taking 4sinθ/λ and βcosθ/λ along x- and y-axis, respectively. By linear fitting the calculated data, the crystallite size and strain is extracted from y-intercepts and slopes of the linear fit lines, respectively. A comparative investigations between crystallite size and strain, calculated from Debye-Scherer's relation, Wilson-stokes relation and W–H plot are given in Figures 3 and 4, respectively. The strain calculated from Wilson–Stokes relation has somehow different values as compared to that calculated by using W–H plot method, which might be due to the involvement of various peaks in W-H plot with different FWHM, therefore, different strain values appear. The most intense (110) peak has been used to calculate strain using Wilson-stokes relation. According to a dislocation model, the defects may induce anisotropic strain with in the crystals, therefore, magnitude of strain may vary for various crystallographic planes and this might be the reason for observed considerable differences in the strain calculated by two methods (Ungar, 2008). The presence of strain indicates the imperfections are present in the fabricated samples, which could either be arising from the film-substrate interface, Ni dopant introducing stresses into the host TiO2 lattice or because of the native ion defects arising because of the employed growth conditions, in which the employed thermal energy is not significantly relieved from the host lattice, and therefore, exerts stresses.

Fig. 4.

The strain calculated from Wilson-stokes relation and W–H analysis is plotted against the Ni content. The observed difference may arise because of the residual anisotropic strain.

(0.12MB).
3.2Surface morphology

The SEM micrographs of Ni-doped TiO2 (xNi=0.00, 0.50, 1.00, 1.50, 2.00 and 2.50 at wt.%) thin films are given in Figure 5. In general, all these thin film samples have exhibited a granular structure. The different nanograins on the surface do not have large size variations. However, a porous structure between different grains is also evident. The calculated grain size decreases from 266.19nm to 222.17nm with increase in Ni concentration (xNi=0.00, 0.50, 1.00, 1.50, 2.00 and 2.50wt.%). We have compared the crystallite size calculated from XRD patterns and the grain size calculated from SEM, for varying Ni content as given in Figure 3. There is a small fluctuation in grain size with increasing Ni content; however it has an overall decreasing tendency. The XRD crystallite size decreases as the Ni content increases above up to xNi=1.00%, further increasing the Ni content reduces the crystallite size. Moreover, the crystallite size calculated from XRD and the Williamson analysis are plotted in Figure 3, in which it is evident that with varying the Ni content a small fluctuation in grain size occurs, as determined from the SEM images. The difference between the crystallite size and grain size variations are due to the fact that both should be considered as independent parameters because an ambiguous relation exists among them. Because, a big grain shown by an SEM image may contain several crystallites, as depicted by XRD studies. The crystallite size extracted using Debye Scherer formula is much smaller than the grain size elucidated from SEM, which is due to the polycrystalline nature of the grown thin film. A grain may be composed of several crystallites because of which, while calculating the average crystallite size using XRD, we sum up all the crystallites contributing to various grains (Hasan & Nasir, 2015). However, we can expect comparable grain and crystallite size if the grown material is single crystalline in nature. Therefore, an obvious relation between both could not be expected (Bushroa, Rahbari, Masjuki, & Muhamad, 2012; Tomaszewski, 2013), and transmission electron microscopy (TEM) investigations can further clarify the relation. The crystallite size calculated from W-H plot and Debye Scherer formulas have a similar trend, which indicates the accuracy of the present work. It has been reported that the surface morphology of TiO2 thin film samples shows columnar grains and roughness of the surface increases with increasing doping (Gültekin, 2014). Similarly, Ahmad MK et al. reported that TiO2 thin films deposited on silicon substrate have smaller pores on the surface, and the grain size increases with increasing the annealing temperature (Ahmad et al., 2010). The evidence of the presence of nanograins, as shown by SEM images, with rutile TiO2 major phase determined by XRD, indicates potential applications of Ni-doped TiO2 thin films in the microelectronic industry.

Fig. 5.

SEM micrographs of undoped and Ni-doped TiO2 thin films deposited on glass substrates. The granular structure along with pores between the grains are present. The measured values of the grain size from the SEM images depict that it decreases continuously as the Ni content in TiO2 thin films is increased.

(0.48MB).
3.3Ferromagnetic properties

The magnetic behaviors of Ni-doped TiO2 thin films are investigated with Vibrating Sample Magnetometer (VSM). The VSM results have shown that ferromagnetic behavior is exhibited by all thin films. The graphs show typical hysteresis loops due to each specimen exhibiting coercivity and remanence, as shown in Figure 6. The diamagnetic effects due to the glass substrates are suppressed by the ferromagnetic signals of the undoped and Ni-doped TiO2 thin films. The hysteresis loops of TiO2 thin films for undoped and doped with xNi=0.50% and xNi=1.00%, shows that in addition to ferromagnetism, there is also a paramagnetic behavior that can be seen from the linear variation of magnetization at higher values of the applied magnetic field. The hysteresis loops of TiO2 thin film doped with xNi=1.50%, xNi=2.00% and xNi=2.50%, shows ferromagnetic behavior, and from these graphs it can be seen that saturation magnetization Msat enhances with Ni content. The values of remanent magnetization Mr, saturation magnetization MS and coercivity Hc of Ni-doped and undoped thin films are listed in Table 2. Remanent magnetization increases continuously up to the sample with xNi=1.50%, however, above this concentration, a sharp increase has been observed. The saturation magnetization decreases up to xNi=2.00% and then a sudden increase appears for TiO2 thin film with xNi=2.50%. The coercivity increases up to the sample with xNi=1.50%, however, it decreases sharply for the samples with xNi=2.00–2.50%, which suggest that Ni-doped TiO2 thin films show soft ferromagnetic behavior at higher Ni concentrations and hard ferromagnetic behavior at lower Ni content, indicating the potential spintronic device applications of TiO2. There are many reports in the literature about the magnetic properties of rutile and anatase phase of TiO2. Recently, Bahadur et al. reported that the magnetic moment of TiNiO2 rises at lower Ni concentrations but with increasing Ni concentration it decreases (Bahadur et al., 2012). The magnetic properties are determined at 300K (room temperature), therefore, the presence of hysteresis even in the undoped TiO2 indicates the presence of room-temperature ferromagnetism (RTFM) (Gao, Tian, Zheng, Tan, & Zhang, 2015), which could be justified by the presence of oxygen interstitial defects. The presence of oxygen defects in the undoped host lattices have already been reported to mediate room-temperature ferromagnetism (Das, Kar, & Srinivasan, 2014). It has already been reported that intrinsic TiO2 is n-type semiconductor, which become p-type because of Ni doping. The n-type to p-type change in character is due to the vacancies introduced by the Ni dopant. In order to determine the real origin of room-temperature ferromagnetism (RTFM) in the studied thin films, we can consider various possible mechanisms. One possibility of the appearance of RTFM is due to the presence of secondary phases (Radovanovic & Gamelin, 2003; Schwartz, Norberg, Nguyen, Parker, & Gamelin, 2003) which could be ruled out, according the XRD that excludes the secondary phase appearance. Another mechanism is the formation of bound magnetic polaron (BMP). It has already been reported that TiO2 exhibits robust polaronic effect. According to BMP, effective mass of carriers is increased because of the sturdy electron-phonon interaction. A trapped electron at an oxygen vacancy causes an F-center, and because of its orbital, it will effectively overlap surrounding Ni ions. Hence the possible mechanism for origin of magnetism in TiO2 is due to the F-center induced BMP, which is mediated by localized electrons, surrounding the impurities (Tian, Gao, Deng, et al., 2013; Tian, Gao, Kong, et al., 2013; Choudhury et al., 2014). Similarly, RKKY model (i.e. the indirect exchange interactions), can also be used to explain the origin causing ferromagnetic behavior in TiO2 host lattice. In RKKY interactions, Ni+2 ions are ferromagnetically coupled through the free carriers (Bahadur et al., 2012).

Fig. 6.

The hysteresis loops measured at 300K for TiO2 thin film doped with xNi=0.50%, 1.00%, 1.50%, 2.00% and xNi=2.50% showing ferromagnetic behavior. The inset figure on the upper left side is plotted around ±2000Oe to observe the details around the origin. The inset figure in the lower right corner shows the hysteresis loop measured for the undoped TiO2 thin film.

(0.39MB).
Table 2.

The remanent magnetization, saturation magnetization and coercivity extracted from the measured hysteresis loops.

xNi
(%) 
Remanent magnetization
(emu/g) 
Saturation magnetization
(emu/g) 
Coercivity
(Oe) 
0.0  4.1E−5  8.16E−4  1079 
0.5  4.4E−5  8.04E−4  1405 
1.0  4.8E−5  6.35E−4  1625 
1.5  4.7E−5  5.37E−4  1675 
2.0  7.9E−5  2.40E−4  0455 
2.5  1.4E−4  11.0E−4  0320 

Transition-metal-doped TiO2 has already been reported to exhibit ferromagnetism mediated by super-exchange d-d mechanism, which increases with increasing dopant concentrations. Therefore, the increase in dopant concentration should result in increase in magnetization of the host lattice, however, a different trend we have found in the studied Ni-doped TiO2 thin films, as evident in Table 2, where up to xNi=2%, remnant magnetization increases but saturation magnetization decreases. As observed in Table 2, the coercivity is higher at smaller dopant concentration, but it decreases at higher Ni content (xNi=2.0–2.5%), indicating a shift of relatively hard to soft ferromagnetic behaviors of the fabricated thin films, which could be associated with the residual strains, as determined from XRD, that can reduce the magnetic anisotropy of the doped TiO2 thin films.

The variation in ferromagnetic characteristics is related with the XRD and SEM studies. By increasing the magnetic impurity concentration in TiO2, there appears no secondary phase belonging to Ni, as depicted in Figure 1, where a major rutile phase of TiO2 thin films appear. This shows that Ni+2 ion replaces Ti+4 ions substitutionally and result in a nearly linear decay of SEM grain size, as is evident in Figure 3. The corresponding magnetic properties also vary linearly, as illustrated by VSM results in Table 2, which is in agreement with the earlier reports that content of added magnetic ions, substituting the host lattice cations, may induce proportional ferromagnetic behavior, in the host lattice (Bahadur et al., 2012; Sabry, Al-Haidarie, & Kudhier, 2016).

4Conclusions

Undoped and Ni-doped TiO2 thin films have successfully been synthesized on glass substrates by a very simple solid-state reaction and dip coating technique. It has been observed that Ni doping plays a vibrant role in the exhibited physical characteristics such as crystal quality, crystallite size and magnetic characteristics of Ni-doped TiO2 thin films. The observed average crystallite size is 17.677nm. Good agreement between values of the crystallite size and strain, extracted from the major XRD peaks and through the W-H analysis, has been found. The surface morphology of all samples elucidated by SEM shows that there is an overall decreasing tendency in nanograin size with increasing Ni content. The average grain size decreases from 266.19nm to 222.17nm with the added Ni content. Room-temperature ferromagnetism (RTFM) is illustrated in the prepared thin films. The measured characteristics of the studied thin films are found to depend upon the Ni content, where it shows hard ferromagnetic behavior up to xNi=1.5% and exhibits soft ferromagnetic trend above xNi=1.5%, therefore, the observed characteristics of Ni-doped TiO2 thin films are tunable by the Ni content and can be employed in various spintronic device applications.

Conflict of interest

The authors have no conflicts of interest to declare.

Acknowledgment

One of the authors, Mahmood-ul-Hassan (M. Hassan), is thankful to University of the Punjab, Lahore, for financial support through order no. D/1384/Est-I.

References
[Ayieko et al., 2013]
C.O. Ayieko, R.J. Musembi, S.M. Waita, B.O. Aduda, P.K. Jain.
Performance of TiO2/In (OH) i S j/Pb (OH)x Sy Composite ETA solar cell fabricated from nitrogen doped TiO2 thin film window layer.
International Journal of Materials Engineering, 3 (2013), pp. 11-16
[Ahmad et al., 2010]
M.K. Ahmad, M.L.M. Halid, N.A. Rasheid, A.Z. Ahmed, S. Abdullah, M. Rusop.
Effect of annealing temperature on surface morphology and electrical properties of TiO2 thin films prepared by sol–gel method.
Journal of Sustainable Energy & Environment, 1 (2010), pp. 17-20
[Akpan and Hameed, 2010]
U.G. Akpan, B.H. Hameed.
The advancements in sol–gel method of doped-TiO2 photocatalysts.
Applied Catalysis A: General, 375 (2010), pp. 1-11
[Al-Jawad, 2014]
S.M.H. Al-Jawad.
Effect of doping on structural and electrical properties of TiO2 thin films for gas sensors.
International Journal of Engineering Science, 5 (2014), pp. 2171-2176
[Asahi et al., 2014]
R. Asahi, T. Morikawa, H. Irie, T. Ohwaki.
Nitrogen-doped titanium dioxide as visible-light-sensitive photocatalyst: Designs, developments, and prospects.
Chemical Reviews, 114 (2014), pp. 9824-9852
[Babu et al., 2016]
S.H. Babu, N.S. Krishna, S. Kaleemulla, N.M. Rao, M. Kuppan, C. Krishnamoorthi, G.A. Basheed.
Synthesis and characterizations of (In0.90Sn0.05Ni0.05)2O3 nanoparticles using solid state reaction method.
AIP conference proceedings (Vol. 1731, No. 1, p. 120003),
[Babu and Kaleemulla, 2016]
S.H. Babu, S. Kaleemulla.
Room temperature ferromagnetism in ITO and Ni doped ITO.
Advanced Materials Letters, 7 (2016), pp. 891-896
[Bahadur et al., 2012]
N. Bahadur, R. Pasricha, Govind, S. Chand, R.K. Kotnala.
Effect of Ni doping on the microstructure and high curie temperature ferromagnetism in Sol–gel derived titania powders.
Materials Chemistry and Physics, 133 (2012), pp. 471-479
[Borges et al., 2012]
P.D. Borges, L.M. Scolfaro, H.W.L. Alves, E.F. da Silva, L.V. Assali.
Study of the oxygen vacancy influence on magnetic properties of Fe-and Co-doped SnO2 diluted alloys.
Nanoscale Research Letters, 7 (2012), pp. 540
[Bushroa et al., 2012]
A.R. Bushroa, R.G. Rahbari, H.H. Masjuki, M.R. Muhamad.
Approximation of crystallite size and microstrain via XRD line broadening analysis in TiSiN thin films.
Vacuum, 86 (2012), pp. 1107-1112
[Buzby et al., 2006]
S. Buzby, M.A. Barakat, H. Lin, C. Ni, S.A. Rykov, J.G. Chen, S.I. Shah.
Visible light photocatalysis with nitrogen doped TiO2 nanoparticles prepared by plasma assisted chemical vapor deposition.
Journal of Vacuum Science & Technology, 24 (2006), pp. 1210-1214
[Chen et al., 2006]
D. Chen, D. Yang, Q. Wang, Z. Jiang.
Effects of boron doping on photocatalytic activity and microstructure of titanium dioxide nanoparticles.
Industrial & Engineering Chemistry Research, 45 (2006), pp. 4110-4116
[Choudhury et al., 2014]
B. Choudhury, R. Verma, A. Choudhury.
Oxygen defect assisted paramagnetic to ferromagnetic conversion in Fe doped TiO2 nanoparticles.
RSC Advances, 4 (2014), pp. 29314-29323
[Das et al., 2014]
A.K. Das, M. Kar, A. Srinivasan.
Room temperature ferromagnetism in undoped ZnO nanofibers prepared by electrospinning.
Physica B: Condensed Matter, 448 (2014), pp. 112-114
[Gao et al., 2015]
H. Gao, J. Tian, H. Zheng, F. Tan, W. Zhang.
Effects of Fe doping on the optical and magnetic properties of TiO2 films deposited on Si substrates by a sol–gel route.
Journal of Sol–Gel Science and Technology, 74 (2015), pp. 521-527
[Gültekin, 2014]
A. Gültekin.
Effect of Au nanoparticles doping on the properties of TiO2 thin films.
Materials Science, 20 (2014), pp. 10-14
[Hamal and Klabunde, 2007]
D.B. Hamal, K.J. Klabunde.
Synthesis, characterization, and visible light activity of new nanoparticle photocatalysts based on silver, carbon, and sulfur-doped TiO2.
Journal of Colloid and Interface Science, 311 (2007), pp. 514-522
[Hasan and Nasir, 2015]
B.A. Hasan, E.M. Nasir.
Structural morphology and electrical properties of vacuum evaporated SnS thin films.
International Journal of Current Engineering and Technology, 5 (2015), pp. 910-917
[Hermawan et al., 2011]
P. Hermawan, H.D. Pranowo, I. Kartini.
Physical characterization of Ni (II) doped TiO2 nanocrystal by sol–gel process.
Indonesian Journal of Chemistry, 11 (2011), pp. 135-139
[Hernández-Martínez et al., 2012]
A.R. Hernández-Martínez, M. Estevez, S. Vargas, F. Quintanilla, R. Rodríguez.
Natural pigment-based dye-sensitized solar cells.
Journal of Applied Research and Technology, 10 (2012), pp. 38-47
[Hong et al., 2006]
N.H. Hong, J. Sakai, N. Poirot, V. Brizé.
Room-temperature ferromagnetism observed in undoped semiconducting and insulating oxide thin films.
Physical Review B, 73 (2006), pp. 132404
[Kuppan et al., 2016a]
M. Kuppan, S. Kaleemulla, N.M. Rao, C. Krishnamoorthi, I. Omkaram, D.S. Reddy.
Microstructure and Magnetic Properties of Sn1−xNixO2 thin films prepared by flash evaporation technique.
Journal of Materials Science: Materials in Electronics, (2016),
(Unpublished manuscript)
[Kuppan et al., 2016b]
M. Kuppan, S. Kaleemulla, N.M. Rao, C. Krishnamoorthi, G.V. Rao, I. Omkaram, D.S. Reddy.
Structural, optical and room temperature ferromagnetic properties of Sn1-xFexO2 thin films using flash evaporation technique.
Journal of Superconductivity and Novel Magnetism, (2016),
(Unpublished manuscript)
[Kuznetsov et al., 2009]
A.Y. Kuznetsov, R. Machado, L.S. Gomes, C.A. Achete, V. Swamy, B.C. Muddle, V. Prakapenka.
Size dependence of rutile TiO2 lattice parameters determined via simultaneous size, strain, and shape modeling.
Applied Physics Letters, 94 (2009), pp. 193117
[Li et al., 2013]
Z. Li, D. Ding, Q. Liu, C. Ning.
Hydrogen sensing with Ni-doped TiO2 nanotubes.
Sensors, 13 (2013), pp. 8393-8402
[Niemela et al., 2014]
J.P. Niemela, H. Yamauchi, M. Karppinen.
Conducting Nb-doped TiO2 thin films fabricated with an atomic layer deposition technique.
Thin solid films, 551 (2014), pp. 19-22
[Nosaka et al., 2005]
Y. Nosaka, M. Matsushita, J. Nishino, A.Y. Nosaka.
Nitrogen-doped titanium dioxide photocatalysts for visible response prepared by using organic compounds.
Science and Technology of Advanced Materials, 6 (2005), pp. 143-148
[Oganisian et al., 2015]
K. Oganisian, A. Hreniak, A. Sikora, D. Gaworska-Koniarek, A. Iwan.
Synthesis of iron doped titanium dioxide by sol–gel method for magnetic applications.
Processing and Application of Ceramics, 9 (2015), pp. 43-51
[Park et al., 2007]
Y.R. Park, S.L. Choi, J.H. Lee, K.J. Kim, C.S. Kim.
Ferromagnetic properties of Ni-doped rutile TiO2−δ.
Journal of the Korean Physical Society, 50 (2007), pp. 638-642
[Patle et al., 2015]
L.B. Patle, P.K. Labhane, V.R. Huse, A.L. Chaudhari.
Structural analysis of Cu doped TiO2 nanoparticles using Williamson–Hall method.
International Journal of Scientific Research in Science, Engineering and Technology, 1 (2015), pp. 66-70
[Paulauskas et al., 2013]
I.E. Paulauskas, D.R. Modeshia, T.T. Ali, E.H. El-Mossalamy, A.Y. Obaid, S.N. Basahel, F.K. Sartain.
Photocatalytic activity of doped and undoped titanium dioxide nanoparticles synthesised by flame spray pyrolysis.
Platinum Metals Review, 57 (2013), pp. 32-43
[Paxton and Thien-Nga, 1998]
A.T. Paxton, L. Thien-Nga.
Electronic structure of reduced titanium dioxide.
Physical Review B, 57 (1998), pp. 1579-1584
[Prabbu et al., 2013]
Y.T. Prabbu, K.V. Rao, V.S.S. Kumar, B.S. Kumari.
X-ray analysis and Williamson- Hall size strain plot methods of ZnO nanoparticles with fuel variation.
World Journal of Nano Science and Engineering, 4 (2013), pp. 21-28
[Purushothan and Krishna, 2015]
E. Purushothan, N.G. Krishna.
X-ray determination of crystallite size and effect of lattice strain on the Debye–Waller factors of Ni nano powders using high energy Ball Mill.
Chemistry and Materials Research, 7 (2015), pp. 1-6
[Radovanovic and Gamelin, 2003]
P.V. Radovanovic, D.R. Gamelin.
High-temperature ferromagnetism in Ni 2+-doped ZnO aggregates prepared from colloidal diluted magnetic semiconductor quantum dots.
Physical Review Letters, 91 (2003), pp. 157202
[Sabry et al., 2016]
R.S. Sabry, Y.K. Al-Haidarie, M.A. Kudhier.
Synthesis and photocatalytic activity of TiO2 nanoparticles prepared by sol–gel method.
Journal of Sol–Gel Science and Technology, 78 (2016), pp. 299-306
[Sahdan et al., 2012]
M.Z. Sahdan, N. Nayan, S.H. Dahlan, M.E. Mahmoud, U. Hashim.
Sol–gel synthesis of TiO2 thin films from in-house nano-TiO2 powder.
Advances in Materials Physics and Chemistry, 2 (2012), pp. 16-20
[Schwartz et al., 2003]
D.A. Schwartz, N.S. Norberg, Q.P. Nguyen, J.M. Parker, D.R. Gamelin.
Magnetic quantum dots: Synthesis, spectroscopy, and magnetism of Co2+-and Ni2+-doped ZnO nanocrystals.
Journal of the American Chemical Society, 125 (2003), pp. 13205-13218
[Seery et al., 2007]
M.K. Seery, R. George, P. Floris, S.C. Pillai.
Silver doped titanium dioxide nanomaterials for enhanced visible light photocatalysis.
Journal of Photochemistry and Photobiology A: Chemistry, 189 (2007), pp. 258-263
[Sobana et al., 2006]
N. Sobana, M. Muruganadham, M. Swaminathan.
Nano-Ag particles doped TiO2 for efficient photodegradation of direct azo dyes.
Journal of Molecular Catalysis A: Chemical, 258 (2006), pp. 124-132
[Tian et al., 2013a]
J. Tian, H. Gao, H. Deng, L. Sun, H. Kong, P. Yang, J. Chu.
Structural, magnetic and optical properties of Ni-doped TiO2 thin films deposited on Si (100) substrates by sol–gel process.
Journal of Alloys and Compounds, 581 (2013), pp. 318-1293
[Tian et al., 2013b]
J. Tian, H. Gao, H. Kong, P. Yang, W. Zhang, J. Chu.
Influence of transition metal doping on the structural, optical and magnetic properties of TiO2 thin films deposited on Si substrate by a sol–gel process.
Nanoscale Research Letters, 8 (2013), pp. 533
[Tomaszewski, 2013]
P.E. Tomaszewski.
The uncertainty in the grain size calculation from X-ray diffraction data.
Phase Transitions, 86 (2013), pp. 260-266
[Ungar, 2008]
T. Ungar.
Dislocation model of strain anisotropy.
Powder Diffraction, 23 (2008), pp. 125-132
[Di Valentin et al., 2005]
C. Di Valentin, G. Pacchioni, A. Selloni.
Theory of carbon doping of titanium dioxide.
Chemistry of Materials, 17 (2005), pp. 6656-6665
[Vijay et al., 2009]
M. Vijay, V. Selvarajan, K.P. Sreekumar, J. Yu, S. Liu, P.V. Ananthapadmanabhan.
Characterization and visible light photocatalytic properties of nanocrystalline TiO2 synthesized by reactive plasma processing.
Solar Energy Materials and Solar Cells, 93 (2009), pp. 1540-1549
[Wilso et al., 2006]
G.J. Wilso, A.S. Matijasevich, D.R. Mitchell, J.C. Schulz, G.D. Will.
Modification of TiO2 for enhanced surface properties: Finite Ostwald ripening by a microwave hydrothermal process.
Langmuir, 22 (2006), pp. 2016-2027
[Yang et al., 2007]
X. Yang, C. Cao, K. Hohn, L. Erickson, R. Maghirang, D. Hamal, K. Klabunde.
Highly visible-light active C-and V-doped TiO2 for degradation of acetaldehyde.
Journal of Catalysis, 252 (2007), pp. 296-302
[Xu et al., 2009]
Y. Xu, Y. Tang, C. Li, G. Cao, W. Ren, H. Xu, Z. Ren.
Synthesis and room-temperature ferromagnetic properties of single-crystalline Co-doped SnO2 nanocrystals via a high magnetic field.
Journal of Alloys and Compounds, 481 (2009), pp. 837-840
[Yoon et al., 2006]
S.D. Yoon, Y. Chen, A. Yang, T.L. Goodrich, X. Zuo, D.A. Arena, V.G. Harris.
Oxygen-defect-induced magnetism to 880K in semiconducting anatase TiO2−δ films.
Journal of Physics: Condensed Matter, 18 (2006), pp. L355

Peer Review under the responsibility of Universidad Nacional Autónoma de México.

Copyright © 2017. Universidad Nacional Autónoma de México, Centro de Ciencias Aplicadas y Desarrollo Tecnológico
Descargar PDF
Opciones de artículo