metricas
covid
Buscar en
Revista Española de Cirugía Ortopédica y Traumatología (English Edition)
Toda la web
Inicio Revista Española de Cirugía Ortopédica y Traumatología (English Edition) Influence of the physiological medium on the mechanical properties of bone cemen...
Información de la revista
Vol. 58. Núm. 1.
Páginas 3-10 (enero - febrero 2014)
Visitas
1703
Vol. 58. Núm. 1.
Páginas 3-10 (enero - febrero 2014)
Research
Acceso a texto completo
Influence of the physiological medium on the mechanical properties of bone cement: Can current studies be extrapolated?
Influencia del medio fisiológico sobre las propiedades mecánicas del cemento óseo. ¿Son los estudios actuales extrapolables?
Visitas
1703
P. Sanz-Ruiza,
Autor para correspondencia
pablo.sanzruiz@gmail.com

Corresponding author.
, E. Pazb, J. Abenojarc, J.C. del Realb, F. Forriold, J. Vaqueroa
a Servicio de Cirugía Ortopédica y Traumatología, Hospital General Universitario Gregorio Marañón, Madrid, Spain
b Instituto para la investigación tecnológica, Departamento de ingeniería mecánica, Universidad Pontificia Comillas, Madrid, Spain
c Grupo desarrollo materiales, Departamento de ingeniería y ciencia de materiales, Universidad Carlos III, Madrid, Spain
d Facultad de Medicina, Universidad San Pablo CEU, Madrid, Spain
Este artículo ha recibido
Información del artículo
Resumen
Texto completo
Bibliografía
Descargar PDF
Estadísticas
Figuras (5)
Mostrar másMostrar menos
Tablas (3)
Table 1. Definition of the 4 groups based on conditioning process.
Table 2. Mean results and standard deviation obtained in wear testing.
Table 3. Mean results and standard deviation obtained in flexion testing.
Mostrar másMostrar menos
Abstract
Purpose

The use of bone cement is widespread in orthopedic surgery. Most of the mechanical tests are performed in dry medium, making it difficult to extrapolate the results. The objective of this study is to assess if the mechanical properties of polymethylmethacrylate (PMMA), obtained in previous reports, are still present in a liquid medium.

Materials and methods

An experimental study was designed with antibiotic (vancomycin) loaded PMMA. Four groups were defined according to the medium (dry or liquid) and the pre-conditioning in liquid medium (one week or one month). Wear and flexural strength tests were performed according to ASTM and ISO standards. Volumetric wear, friction coefficient, tensile strength, and Young's modulus were analyzed. All samples were examined by scanning electron microscopy.

Results

The samples tested in liquid medium showed lower wear and flexural strength values (P<.05). The kind of wear was modified from abrasive to adhesive in those samples studied in liquid medium. The samples with a pre-conditioning time showed lower values of wear (P<.05).

Conclusions

Caution is recommended when extrapolating the results of previous PMMA results. The different mechanical strength of the cement in a liquid medium, observed in saline medium, is much closer to the clinical situation.

Keywords:
Polymethylmethacrylate
Bone cement
Antibiotic loaded cement
Periprosthetic infection
Resumen
Objetivo

El uso del cemento óseo esta muy extendido en COT, existiendo multitud de estudios experimentales que lo avalan. La mayoría de los ensayos mecánicos están realizados en seco, lo que cuestiona la extrapolación de los resultados a la clínica. El objetivo de este estudio es evaluar si las propiedades mecánicas del polimetilmetacrilato (PMMA) obtenidas en series previas en seco, se mantienen en un medio fisiológico.

Material y método

Se ha diseñado un estudio experimental para evaluar este aspecto, utilizando PMMA con antibiótico (vancomicina). Cuatro grupos fueron definidos en función del medio estudiado (seco o líquido) y de la realización de un acondicionamiento previo en suero fisiológico (una semana o un mes). Se hicieron estudios de desgaste y resistencia a flexión según las normativas ISO y ASTM, valorando el desgaste, el coeficiente de fricción, la resistencia a la rotura y el modulo de Young. Las muestras fueron analizadas mediante microscopía electrónica.

Resultados

Las muestras ensayadas en medio líquido presentaron menores valores de desgaste, así como menor resistencia a flexión, obteniéndose significación en el desgaste. El tipo de desgaste se modificó de un desgaste abrasivo a uno adhesivo en aquellas muestras estudiadas en medio líquido. El tiempo de acondicionamiento proporcionó menores valores de desgaste (P<0,05).

Conclusiones

Se recomienda precaución a la hora de extrapolar los resultados de los estudios sobre PMMA en seco dado el diferente comportamiento mecánico del cemento en un medio líquido mucho más cercano a la situación clínica real, como es el suero fisiológico.

Palabras clave:
Polimetilmetacrilato
Cemento óseo
Cemento con antibiótico
Infección protésica
Texto completo
Introduction

Since the use of polymethylmethacrylate (PMMA) by Dr. Charnley in the 1960s as a method of fixation for hip arthroplasties,1,2 PMMA has been shown to be one of the best methods of implant fixation in orthopedic surgery, with survival rates of more than 90% at 15 years in knee4 and hip3 arthroplasties. In addition to its usefulness in fixation, PMMA has been shown to be the best vehicle to date for using high amounts of antibiotics in the treatment of osteoarticular infection (and especially in prosthetic infection), achieving high local concentrations with very few systemic effects. This is particularly important, given that an increase of nearly 50% in the rate of prosthesis review caused by infection is projected by 2030.5

The usefulness of PMMA as a method of fixation, as well as growing interest in its use in the treatment and prophylaxis of prosthetic infection, has made it into one of the most frequently studied materials in our environment; this in turn has led to the appearance of multiple commercial preparations and the publication of minimum requirements by international agencies such as the ISO and the ASTM.6–8 Given that the great majority of studies performed to date have been under experimental conditions of dry medium, it is difficult to extrapolate these results correctly to clinical practice. This difficulty undoubtedly is of special interest when studying PMMA used with antibiotics, whose elution in liquid medium inevitably affects the mechanical characteristics of PMMA.

The objective of this study was to assess the influence of a liquid medium such as saline solution on the resistance and wear of bone cement mixed with an antibiotic, and whether such influence varied over time.

Materials and methods

We performed an experimental study to assess the effect on liquid medium on bone cement. The PMMA used was bone cement that was quick setting, of high viscosity and preloaded with 0.5g of gentamicin Palacos® R+G (Heraeus Medical GmbH, Wehrheim, Germany), because of its wide use and its good survival data in various series.9,10 To each commercial preparation of cement, we added a vial of 1g of powdered vancomycin (Normon EFG, Tres Cantos, Madrid, Spain) manually to reproduce the treatment conditions of an infected arthroplasty.

Two types of samples were prepared: circular and rectangular. Before sample preparation the cement had been stored at controlled temperature and relative humidity. The components were not cooled beforehand; they were mixed in a tray manually. We added vancomycin independently, following the method of Frommelt and Kühn11 for manual addition of antibiotics, previously adding the same amount of powdered antibiotic as of polymer in a tray for a minute until we achieved a homogeneous mixture of the powder. Room temperature at the time of mixing was 23°C, with a relative humidity of 55–60%. The mixing process was carried out following the recommendation of the manufacturer and ASTM F451-996 and ISO 5833:20028 regulations. Each 20-ml vial of monomer was mixed with a 40-g sachet of polymer, added in that order in a reusable plastic tray. The mixture was prepared by stirring in a clock-wise direction in homogeneous frequency for a timed period of 30s. Once the paste was achieved, it was left to set until it was shown that the mixture would not stick (2min at work temperature), then beginning the preparation of the samples.

To prepare the samples we used a predesigned mold made of silicone (Fig. 1A and B), with circular samples 30mm in diameter and 4mm thick (Fig. 1C) and rectangular samples 79mm long, 10mm wide and 4.5mm high (Fig. 1D). The process of preparing these was similar, using cement in ductile phase to fill the molds, leaving them to set under a continuous weight of 10kg to become compact and to obtain homogeneous samples. Following a hardening period (10–12min) we removed the samples from the molds. Each bag of cement yielded enough for the preparation of 6 samples in 1 of the molds. The circular samples were used to study wear, while the rectangular ones were used to study resistance to fracture.

Figure 1.

Molds used to prepare the samples of wear (A) and flexion (B). Samples before their testing, once removed from the mold (C and D).

(0.11MB).

We defined various groups based on the conditioning process to which they were submitted, yielding 4 groups for the circular samples and 2 groups for the rectangular samples (Table 1). The conditioning process consisted of immersing the samples in isotonic saline solution (B. Braun, Melsungen, Germany) during the appropriate time for each group, maintaining the samples at a constant temperature of 37°C by incubation with a heater. These conditions attempted to replicate a medium similar to that which exists in a joint. Three homogeneous samples were prepared for each study group.

Table 1.

Definition of the 4 groups based on conditioning process.

  Circular samples  Rectangular samples 
Group 1  No conditioning. Samples tested in dry medium  No conditioning. Samples tested in dry medium 
Group 2  Samples tested in liquid medium without prior conditioning  – 
Group 3  Samples tested in liquid medium after a week of conditioning  – 
Group 4  Samples tested in liquid medium after a month of conditioning  Samples tested in liquid medium after a month of conditioning 

For the determination of wear and of the coefficient of friction, we performed mechanical testing following Standard ASTM G99-05.7 For the production of a wear track, we used a PIN-ON-DISK tribometer (Microtest, Madrid, Spain), with a 304 stainless steel ball 6mm in diameter. The test conditions used were with a normal load applied of 15N, a described path of 1000m, and a frequency of 120rpm (Fig. 2B and D). For the tests performed with the samples submerged in saline solution, a recipient was attached to the tribometer plate, where the samples covered in saline solution were introduced. The measurement of the wear track and its width was done with a V-20A Nikon Profile Projector (Nikon instrument INT, NY, USA). The use of a trigonometric model let us measure the wear obtained, defining the volume lost in mm3/Nm (Fig. 3). All of the samples tested were observed using a scanning electron microscope, with a previous requisite gold dust coated by sputtering.

Figure 2.

Instruments used to carry out the testing and the conditions applied. Universal testing machine (A) and tribometer (B). Illustration of the study conditions for flexion (C) and wear (D) testing.

(0.35MB).
Figure 3.

Trigonometric model used to calculate wear; d (distance covered=1000m), F (force applied=15N), Vlost (volume lost due to wear), Vtorus (volume of the rotation torus), Rspin (radius of the wear track), Rball (radius of the wear ball=6mm), Dexternal (external diameter of the wear track), B (width of the track), A (area), and h (height).

(0.1MB).

To assess the resistance of the samples at a moment of flexion, we carried out testing using the international standard ISO 178:1993 and its Spanish modification UNE-EN-ISO 178. We used a universal testing machine (IB-MU4, IBERTEST, Ibertest group, Madrid, Spain) with 3-point flexion testing jaws, placing each sample over the lower points and applying a central force over the upper face of the sample. The distance between both lower supports was 64mm, applying the force in the central point at a speed of 1mm/min (Fig. 2A and C).

For the statistical analysis, we used the SPSS® version 15.0 computer package for MS-Windows (SPSS Inc., Chicago, USA). The ANOVA test was used for the comparison of the variables studied among the various groups for the wear tests, and Student's t-test for independent samples in the mechanical resistance studies. Statistically significant differences were defined as those having P values lower than 5% (P<.05).

Results

Table 2 shows the results obtained in the wear testing. In the samples tested in dry medium there were wear and coefficient of friction values significantly greater than those tested in liquid medium, whatever the process of conditioning (P<.05). The medium of study also conditioned how wear was produced, in that continuous wear was observed in the samples in dry medium in comparison to exponential wear in samples studied in liquid medium (Fig. 4). The decrease in wear observed was more than 60% (Table 2). The performance of a previous process of conditioning (Groups 3–4) diminished both wear and the coefficient of friction obtained in comparison to the samples that presented a lack of conditioning (Group 2), although there was no statistically significant difference. Increasing the time of conditioning from 1 week (Group 3) to 1 month (Group 4) produced a significantly greater decrease in the values of wear and coefficient of friction (P=.04).

Table 2.

Mean results and standard deviation obtained in wear testing.

  Group 1Dry medium without conditioning  Group 2Liquid medium without conditioning  Group 3Liquid medium 1 week of conditioning  Group 4Liquid medium 1 month of conditioning 
Wear track width  1.20±0.02mm  0.86±0.01mm  0.83±0.02mm  0.73±0.01mm 
Wear track diameter  17.59±0.8mm  17.94±0.9mm  18.82±0.1mm  18.70±0.1mm 
Wear  0.09±0.09mm3/Nm×10−4  0.03±0.003mm3/Nm×10−4  0.03±0.003mm3/Nm×10−4  0.02±0.001mm3/Nm×10−4 
Coefficient of friction  0.72±0.07  0.49±0.08  0.44±0.05  0.36±0.08 
Figure 4.

Evolution of the coefficient of friction in liquid medium (upper figure) and in dry medium (lower figure).

(0.18MB).

Scanning electron microscopy (SEM) showed a smaller size of the wear tracks tested in dry medium. The wear was of the abrasive type, changing to mainly adhesive when testing the samples in liquid medium (Fig. 5).

Figure 5.

Images of the wear tracks obtained by electron microscope. In the upper images (A–C) abrasive wear can be seen in contrast to that obtained in the lower images (D–F). Note the particles adhered to the surface in E and (in a larger scale) in Image F.

(0.34MB).

The results obtained in the flexion testing are summarized in Table 3. Samples tested in liquid medium presented lower resistance to breaking, bearing forces of lesser magnitude and suffering deformation to a lesser degree, than the samples studied in dry medium. The stress registered in the samples studied in liquid medium was also lower than that obtained in dry medium. No variations in the model of elasticity were observed.

Table 3.

Mean results and standard deviation obtained in flexion testing.

  Dry medium (no conditioning)  Liquid medium (1 month of conditioning) 
Max. force  0.09±0.01kN  0.06±0.045kN 
Max. stress  46.3±2.3MPa  42.5±2.7MPa 
Max. deformation  0.04±0.02mm  0.03±0.005mm 
Young model  1814.9±71.3  1819.7±64.5 
Discussion

The results of our study were influenced by the choices of bone cement, environmental conditions, and antibiotic. For this study we used Palacos® R+G (Heraeus Medical GmbH, Wehrheim, Germany) as it is one of the most widely used commercial cements that had the best long-term results.12,13 The environmental conditions selected were defined attempting to imitate the normal conditions existing in operating rooms where bone cement is used.14,15 The industrial addition of a small amount of an antibiotic like gentamicin has not been shown to affect the mechanical properties in previous studies.16 The choice of vancomycin as the antibiotic was based on its wide distribution, its use as treatment of prosthesis infection associated to PMMA, and its reduced price.9,17 All samples were mixed manually. This method increases porosity in PMMA, which leads to reducing the mechanical resistance and increasing the elution of PMMA.3,18–20 This has been called into question by McLaren et al.21

The effect of immersing PMMA in a liquid medium has been studied previously. Schmitt et al. described an increase in cement mass when it was submerged in saline solution.22 Other authors observed a decrease in the model of elasticity as water was absorbed,23 with PMMA even becoming saturated at 3 months without any observable changes in its properties although the water acted as an initiator of fractures.24 The plasticizing effect of the water and its influence on the mechanical properties of the bone cement have been described in detail,22,24,25 with it being due to the absorption of water by the PMMA, a process described in other polymers,26 being cyclic.

In our study we did not find statistical significance in the changes observed in the mechanical properties of PMMA studied in dry medium as compared to that studied in liquid medium. However, there was a clear tendency to a decrease in these properties when we introduced the PMMA in a medium with liquid. These results are the same as those found in the literature. Nottrott27 studied the behavior of Palacos® R+G and CMW 3 Genta® stored for 5 years in a dry medium against for 3 weeks in a medium with water; they found an increase in resistance to stress and in the model of elasticity in the samples that had been stored dry.

The wear observed in our study was low compared to the coefficients of friction obtained, with significantly lower wear in the samples studied in liquid medium. This could be due to the lubricating effect of water, the modification of the wear pattern from an abrasive behavior to an adhesive one, and to the deposit itself of substances in the wear track of the samples tested in liquid (Fig. 5A–F), although the authors have no knowledge of any prior descriptions of this phenomenon.

Bone cement is not a static component; its mechanical properties vary over time. Cizmecioglu et al.28 described the influence of PMMA “aging” on its elasticity, determined by the amount of residual monomer, which has a damaging effect on PMMA resistance.29 In our study, we obtained less wear in the samples that had undergone a process of conditioning, observing an influence of period of adaptation in this decrease; the samples submitted to a month of conditioning presented significantly less wear than the samples submitted to a week. To the best of our knowledge, there is no previous study that evaluates the time of aging in a liquid medium on PMMA resistance to wear.

In contrast to previous studies in the literature, in our study we used PMMA wear as another variable to measure the influence of the liquid medium on mechanical properties. An increase in wear could be prejudicial to implant fixation; Saleh et al.30 and Goodman31 described how the particles of bone cement wear could be involved in periprosthetic osteolysis, although excessive wear could be useful in other situations because of the increase in elution of antibiotic present on the surface of articulating spacers. This study is an initial step in attempting to understand what happens on the surface of these spacers.

In our study we wanted to imitate the environmental conditions in a joint. To this end, we used a medium of study with saline solution, but we must accept certain limitations. A healthy joint contains, in addition to synovial liquid, various substances such as proteins, cells, glucose and so on that give it different rheological properties from those of saline solution. Using a watertight medium for producing the conditioning and wear also differs from the normal behavior of a joint, where there is a flux between absorption/production, in addition to movement, which can have an effect on the particles of wear being deposited on the cement itself and can consequently change the wear values obtained. We feel that it is important to keep these considerations in mind when interpreting the results. We do not believe that the limited number of samples represents a limitation for the results of this study, although it could indeed have limited the obtaining of statistical significance in specific groups. Other publication of special relevance in biomaterials have used similar sample sizes; examples are Unemori et al.25 who utilized 3 samples to observe the absorption of water in modified PMMA, and Bridgens et al.32 who used 2 samples to study the elution and mechanical resistance of various cements mixed with PMMA.

In conclusion, the results obtained in this study show the damaging effect of the liquid medium on PMMA, which brings into question the use of the data obtained in previous studies carried out in dry medium extrapolated to clinical practice. Nevertheless, further studies that back this up are required, as well as additional studies to evaluate if the decrease in PMMA resistance and wear with vancomycin observed in this study continues in other PMMA isolated or in combination with other antibiotics.

Level of evidence

Level of evidence 1.

Ethical responsibilitiesProtection of persons and animals

The authors declare that no experiments on human beings or animals were performed for this research.

Data confidentiality

The authors declare that no patient data appear in this article.

Right to privacy and informed consent

The authors declare that no patient data appear in this article.

Conflicts of interest

The authors have no conflicts of interest to declare.

References
[1]
J. Charnley.
Arthroplasty of the hip. A new operation.
Lancet, 1 (1961), pp. 1129-1132
[2]
J. Charnley.
Anchorage of the femoral head prosthesis to the shaft of the femur.
J Bone Joint Surg Br, 42B (1960), pp. 28-30
[3]
T. Jaeblon.
Polymethylmethacrylate: properties and contemporary uses in orthopaedics.
J Am Acad Orthop Surg, 18 (2010), pp. 297-305
[4]
J.A. Rand, R.T. Trousdale, D.M. Ilstrup, W.S. Harmsen.
Factors affecting the durability of primary total knee prostheses.
J Bone Joint Surg Am, 85A (2003), pp. 259-265
[5]
S.M. Kurtz, K.L. Ong, J. Schmier, F. Mowat, K. Saleh, E. Dybvik, et al.
Future clinical and economic impact of revision total hip and knee arthroplasty.
J Bone Joint Surg Am, 89 (2007), pp. S144-S151
[6]
451-99a American Society for Testing and Materials (ASTM) Standard.
ASTM International, (2007),
[7]
American Society for Testing and Materials (ASTM) Standard G 99-05.
ASTM International, (2010),
[8]
International Standards Organization (ISO).
ISO 5833: implants for surgery-acrylic resin cements. Annex F. Method for determination of bending modulus and strength of cement.
ISO Geneve, (2002),
[9]
A.D. Hanssen, M.J. Spangehl.
Practical applications of antibiotic-loaded bone cement for treatment of infected joint replacements.
Clin Orthop Relat Res, (2004), pp. 79-85
[10]
M.J. Penner, B.A. Masri, C.P. Duncan.
Elution characteristics of vancomycin and tobramycin combined in acrylic bone-cement.
J Arthroplasty, 11 (1996), pp. 939-944
[11]
L. Frommelt, K.-D. Kühn.
Properties of bone cement: antibiotic-loaded cement.
The well-ceemnted total hip arthroplasty, pp. 86-92
[12]
R. De Santis, F. Mollica, L. Ambrosio, L. Nicolais, D. Ronca.
Dynamic mechanical behavior of PMMA based bone cements in wet environment.
J Mater Sci Mater Med, 14 (2003), pp. 583-594
[13]
J.C. Webb, R.F. Spencer.
The role of polymethylmethacrylate bone cement in modern orthopaedic surgery.
J Bone Joint Surg Br, 89B (2007), pp. 851-857
[14]
A.S. Carlsson, J.A. Nilsson, G. Blomgren, G. Josefsson, L.T. Lindberg, R. Onnerfalt.
Low- vs high-viscosity cement in hip arthroplasty. No radiographic difference in 226 arthrosis cases followed for 5 years.
Acta Orthop Scand, 64 (1993), pp. 257-262
[15]
S. Smeds, D. Goertzen, I. Ivarsson.
Influence of temperature and vacuum mixing on bone cement properties.
Clin Orthop Relat Res, 334 (1997), pp. 326-334
[16]
B. Espehaug, L.B. Engesaeter, S.E. Vollset, L.I. Havelin, N. Langeland.
Antibiotic prophylaxis in total hip arthroplasty. Review of 10,905 primary cemented total hip replacements reported to the Norwegian arthroplasty register, 1987 to 1995.
J Bone Joint Surg Br, 79B (1997), pp. 590-595
[17]
W.A. Jiranek, A.D. Hanssen, A.S. Greenwald.
Antibiotic-loaded bone cement for infection prophylaxis in total joint replacement.
J Bone Joint Surg Am, 88 (2006), pp. 2487-2500
[18]
G. Lewis, S. Janna, A. Bhattaram.
Influence of the method of blending an antibiotic powder with an acrylic bone cement powder on physical, mechanical, and thermal properties of the cured cement.
Biomaterials, 26 (2005), pp. 4317-4325
[19]
K.J. Messick, M.A. Miller, L.A. Damron, A. Race, M.T. Clarke, K.A. Mann.
Vacuum-mixing cement does not decrease overall porosity in cemented femoral stems: an in vitro laboratory investigation.
J Bone Joint Surg Br, 89 (2007), pp. 1115-1121
[20]
J. Meyer, G. Piller, C.A. Spiegel, S. Hetzel, M. Squire.
Vacuum-mixing significantly changes antibiotic elution characteristics of commercially available antibiotic-impregnated bone cements.
J Bone Joint Surg Am, 93 (2011), pp. 2049-2056
[21]
A.C. McLaren, M. Nugent, K. Economopoulos, H. Kaul, B.L. Vernon, R. McLemore.
Hand-mixed and premixed antibiotic-loaded bone cement have similar homogeneity.
Clin Orthop Relat Res, 467 (2009), pp. 1693-1698
[22]
S. Schmitt, D.J. Krzypow, C.M. Rimnac.
The effect of moisture absorption on the fatigue crack propagation resistance of acrylic bone cement.
Biomed Technol (Berl), 49 (2004), pp. 61-65
[23]
C.H.Y. Ishiyama.
Effects of humidity on Young's modulus in poly(methyl methacrylate).
J Polym Sci B: Polym Phys, 40 (2002), pp. 460-465
[24]
A. Akashi, Y. Matsuya, M. Unemori, A. Akamine.
The relationship between water absorption characteristics and the mechanical strength of resin-modified glass-ionomer cements in long-term water storage.
Biomaterials, 20 (1999), pp. 1573-1578
[25]
M. Unemori, Y. Matsuya, S. Matsuya, A. Akashi, A. Akamine.
Water absorption of poly(methyl methacrylate) containing 4-methacryloxyethyl trimellitic anhydride.
Biomaterials, 24 (2003), pp. 1381-1387
[26]
J. Abenojar, M. Martínez, F. Velasco, J.C. del Real.
Effect of moisture and temperature on the mechanical properties of an epoxy reinforced with boron carbide.
J Adhes Sci Technol, 24 (2011), pp. 2445-2460
[27]
M. Nottrott.
Acrylic bone cements: influence of time and environment on physical properties.
Acta Orthop Suppl, 81 (2010), pp. 1-27
[28]
M. Cizmecioglu, R.F. Fedors, S.D. Hong, J. Moacanin.
Effect of physical aging on stress relaxation of poly(methyl methacrylate).
Polym Eng Sci, 21 (1981), pp. 940-942
[29]
C.I. Vallo, G.A. Abraham, T.R. Cuadrado, J. San Roman.
Influence of cross-linked PMMA beads on the mechanical behavior of self-curing acrylic cements.
J Biomed Mater Res B: Appl Biomater, 70 (2004), pp. 407-416
[30]
K.J. Saleh, I. Thongtrangan, E.M. Schwarz.
Osteolysis: medical and surgical approaches.
Clin Orthop Relat Res, (2004), pp. 138-147
[31]
S. Goodman.
Wear particulate and osteolysis.
Orthop Clin N Am, 36 (2005), pp. 41-48
[32]
J. Bridgens, S. Davies, L. Tilley, P. Norman, I. Stockley.
Orthopaedic bone cement: do we know what we are using.
J Bone Joint Surg Br, 90 (2008), pp. 643-647

Please cite this article as: Sanz-Ruiz P, Paz E, Abenojar J, del Real JC, Forriol F, Vaquero J. Influencia del medio fisiológico sobre las propiedades mecánicas del cemento óseo. ¿Son los estudios actuales extrapolables?. Rev Esp Cir Ortop Traumatol. 2014;58:3–10.

This study received the 2013 SECOT Award for Basic Research in Orthopedic Surgery and Traumatology.

Copyright © 2013. SECOT
Descargar PDF
Opciones de artículo
es en pt

¿Es usted profesional sanitario apto para prescribir o dispensar medicamentos?

Are you a health professional able to prescribe or dispense drugs?

Você é um profissional de saúde habilitado a prescrever ou dispensar medicamentos

Quizás le interese:
10.1016/j.recote.2021.04.009
No mostrar más